The Quality Management System (ISO 9001:2000) enables ELASTRON KIMYA supplies Thermoplastic Elastomer(TPE) products with the most convenient conditions and best customer satisfaction. The latest development is the certification of Elastron according to ISO 14001:2004 Environmental Management System, which reflects our strong sensitivity to the environment.

Troubleshooting

ELASTRON EXTRUSION TROUBLESHOOTING GUIDE

Problem

Solution

Flow Lines Along
(Extrusion direction)
Increase head/die temperature
Increase screen pack
Clean the screen and the die
Flow Lines Across
Increase barrel temperature
Increase head/die temperature
Use higher L/D extruder
Increase compression ratio
Increase haul off speed
Uneven Cross section
Decrease head/die temperature
Decrease the capacity / throughput
Use screw with longer feed / meeting section
Discolouring
Decrease melt temperature
Decrease head/die temperature
Decrease screw speed
Decrease compression ratio
Purge and clean the machine
Porosity / Splash marks
Pre-dry pellets
Decrease barrel temperature
Use lower shear screw
Apply vacuum vent
Decrease the screw speed
Dull / matt surface
Increase head/die temperature
Increase melt temperature
Increase compression ratio
Low output
Increase head/die temperature
Increase melt temperature
Increase screw speed
Decrease compression ratio
Pre-dry pellets
Decrease screen pack
Poor or no adhesion in co-extrusion
Use a suitable mould for co-extrusion
Increase head/die temperature
Increase melt temperature
Increase die compression